Showing posts with label cracks in hemp walls. Show all posts
Showing posts with label cracks in hemp walls. Show all posts

Thursday, 11 October 2012

Mix too wet

Half way through the hemp walls it was a real blow to our confidence and morale to find out that our hemp mixes have been too wet. Correspondence with Klara from the Australian Hemp Masonry Company pointed to my cracking and pulling away cracking problems being caused by my mixes being too wet and therefore having a higher amount of shrinkage and also possibly insufficient wetting down between layers. On reflection I have noticed that I have been making wetter mixes as the days have got much hotter.

So we have reduced the amount of water in our mix to one 9 litre bucket for each mix (5.5kg hemp, 9kg binder and 8.5kg sand) with just a tiny bit more water added if the sand is really dry. With our dryer mix recipe in hand we did one days work hemping and will be more cautious and see how it goes before doing more walls. We used 9 litres of water only for these mixes and I was worried that they looked too dry as the sand did not seem to be held to the hemp and binder but looked like it was sitting on the outside, but as my partner pointed out I got it wrong the first time, so he got his way and we used 9 litres only. But just to check I made our last mix using 10 litres of water and was much happier with how the sand was bound in.

The dryer mixes looked a little different. They stuck more around the top of the mixer, but when emptied out left the inside of the mixer looking cleaner, they poured out of the buckets easier, but were not any different to tamp.

When I took the form work off these dryer sections the next day I could hear some sand fall out when I removed the formwork, and had a little bit of hemp fall out when I removed the spacers. I thought the wall was well tamped but the hemp falling out happened on a few but not all spacers, so whether it was due to insufficient tamping or too dry a mix I could not tell. To try to ensure more even wetting down, particularly when starting a new rise, where the old layer can be quite dry we have used a children's watering can. Due to other commitments we can not work on the walls for a couple of weeks, so we will see how they look when we return to site by which time they will have had a chance to dry out.
The dryer mix
My friend Martin, who helped out with the build a few weeks ago but has no background in hemp building, seemed to be able to pick the cause of my problems and commented in response to my complaint about cracks in my walls -  "They look like the shallow, narrow, non-structural cracks that you get in cement as it drys, if you mix it up a bit too wet. Isn't that what the render is for? To cover up the imperfections and hold the whole show together?" I only hope he is right about the render being able to cover up such imperfections.

Following my worries about my mix now being too dry, I turned to Klara again for advice. She said "The mix should be as dry as it can be and still clump together." But if with 9 litres of water the mix was still too dry I could add up to a quarter of a bucket of water. So after my earlier debate with my partner it appears that the mix I used with 10 litres is still within the acceptable limits. I estimate that in the old mixes I was using about 12 to 14 litres of water (as my one bucket then was about 4-5 cm from the top), so clearly that was too much water.  

We will finish the rest of the house using dryer mixes and then see what we can do about the back section with the cracks, perhaps we will do some test render patches to see if that will cover them, before we contemplate the possibility of having to pull some sections down and redo them.

Kitchen wall up to window height
Uneven layer due to noggins alternately being at differnt heights at top of previous rise
No new wall, but formwork moved up ready for the next weekend of work

Tuesday, 9 October 2012

Hemp Wall Cracks and Problems

We had a long weekend ahead of us and so started with the most time consuming and difficult part, working in the section above the windows and below the roof. The section we did above the windows did not work as well as hoped. On the outside it was OK, but on the inside where the timber we had added to support the hemp was thicker, we had not left a large enough section to be able to fit our fingers in to tamp the hemp down and accordingly there was insufficient hemp coverage in these sections. We will patch them and hope that the render covers it all evenly.

Insufficient hemp coverage
A patched up section
My second issue was that as the walls have dried they have pulled away from the timber frame at the doors.  I believe that this has been exacerbated by the large number of studs next to some of the doors, up to four studs together. The high walls and large openings for the sliding doors required additional support, hence the high number of studs. I am worried that these sections where the hemp has not been able to key into the other side may crack off. I do not know if such concerns are unwarranted as these edges are bound to the rest of the wall which is keys in to each side. Interestingly at the windows where the hemp is bound into the rest of the wall at the top and bottom the same sort of pulling away has not occurred.

The worst of the pulling away sections
My third problem is a number of cracks, a number of horizontal cracks have developed mostly where two rises join together. There has sometimes been a few weeks between when rises were done, hence the older sections were much dryer. Vertical cracks have also developed on each end of the back pavilion on the shorter walls just around the corner from the long 9.6m back wall. There is one crack in almost an identical position on each of the shorter walls, but no vertical cracks in the long 9.6m wall. Traditionally in a brick wall an expansion joint would be put in a long wall to avoid cracking, but here the cracks have appeared in the shorter walls.

Horizontal crack between layers
Another horizontal crack between two layers of different dryness
Vertical crack
To cope with the pulling away at the door frames I improvised a U-shaped metal bracket out of some left over fascia brackets. The metal, being much thinner than timber restraints, was spaced to ensure that I was still able to tamp all around the bracket. Whether this will work will only be seen once the walls dry out.

Metal bracket placed where there are four studs in a row
Metal bracket inside form work, with enough space left to tamp around it
On the positive side the plumbing rough in had been completed - on the first day my plumber got back from holidays (many thanks). The kitchen wall certainly had a lot of pipes and conduit through it  - hot and cold water, gas and electricity.

Kitchen wall with lots of pipes
Holes made in form work for pipe penetrations
Predicted poor weather over the long weekend did not arrive and we did four days of hemp walling, with Tony once again helping us on the last two days. A third person made the hemp walling more than 50% faster, particularly on the low long easy runs where we quickly went through a lot of mixes. With all this effort we have now started all the walls except a few short ones beside the front door and between the glass sliding doors. To be able to do this we had to relocate two and a half of binder that were too close to the wall in the front pavilion to allow access. Almost one pallet was moved to and stacked up in the room we mix in and the other pallet was stacked extra high on top of the remaining two pallets in the front room. Storage of materials under cover of the roof, while allowing access to the walls has been an issue, solved with the hemp by using up half a bag until it was light enough for two people to lift up onto the other bags, therefore allowing us to clear the floor area quicker than if we had just used full bags.

Back wall of the back pavilion completed
Hemping around the instantaneous gas hot water system
First rise in the kitchen wall
First rise in the front pavilion